Filament Atlas

PLA blend

9 products from 5 makers. Most documented first. Select a column to sort, a product to see its values, print settings and documents.

Key

How the numbers are worked out

BigRep PRO HTStrength XY, MPa45Modulus XY, GPa3.1Charpy notched, kJ/m²8HDT 0.45, °C61HDT 1.8, °C—Price, CAD/kg—Nozzle, °C190–230Bed, °C50–70Chamber, °C—Drying, °C, h504–6 h

BigRep PRO HTBigRep

Only 2.85 mm filament was found; the H2C takes 1.75 mm.

Published values

PropertyAs publishedConditionsOn the Overview
BigRep, FILAMENT PRO HT10 valuesUnless a row says otherwise: specimen not stated
Tensile modulus orientation not stated3100 MPap. 1: Tensile Modulus (ISO 527)ISO 527not in the median: set apart (never used to pass), test bar not described as printed
Tensile strength (yield or break not stated) orientation not stated45 MPap. 1: Tensile Strength (ISO 527)ISO 527not in the median: set apart (never used to pass), test bar not described as printed
Flexural modulus orientation not stated3000 MPap. 1: Flexural Modulus (ISO 178)ISO 178not in the median: set apart (never used to pass), test bar not described as printed
Flexural strength orientation not stated60 MPap. 1: Flexural Strength (ISO 178)ISO 178not in the median: set apart (never used to pass), test bar not described as printed
Charpy impact strength8 kJ/m²p. 1: Impact Strength, Notched (ISO 179)ISO 179not in the median: set apart (never used to pass), test bar not described as printed
HDT at 0.45 MPa61 °Cp. 1: HDT B - 0.45 MPa (ISO 75)
ISO 75As the sheet prints it: ISO 75; 0.45 MPa; method=B
not in the median: set apart (never used to pass), test bar not described as printed
Glass transition temperature60 °Cp. 1: Glass Transition Temperature (Tg) (DSC)
DSCAs the sheet prints it: DSC; method=DSC
in the median
Vicat softening temperature116 °Cp. 1: Vicat Softening Temperature (ISO 306)ISO 306
Melting temperature170 °Cp. 1: Melting Temperature (Tm) (DSC)
DSCAs the sheet prints it: DSC; method=DSC
Density1.3 g/cm³p. 1: Density (ISO 1183)ISO 1183
BigRep, PRO HT Filament - Versatile 3D Printing Material | BigRep1 value
Charpy impact strength orientation not stated8 kJ/m²p. 1: Impact Strength, Notched (ISO 179)ISO 179not in the median: another value of this product is in it

Print settings

Nozzle
190–230 °Cown data sheet
Bed
50–70 °Cown data sheet
Heated chamber
not stated
Drying
50 °C for 4–6 hown data sheet
Hardened nozzle
not stated
Its 2 print profiles, in the documents' words
What the maker says (15)
BigRep HI-TEMPStrength XY, MPa50Modulus XY, GPa4.4Charpy notched, kJ/m²4HDT 0.45, °C58HDT 1.8, °C54Price, CAD/kg—Nozzle, °C190–230Bed, °C50–70Chamber, °C—Drying, °C, h504–6 h

BigRep HI-TEMPBigRep

Only 2.85 mm filament was found; the H2C takes 1.75 mm.

Published values

PropertyAs publishedConditionsOn the Overview
BigRep, HI-TEMP filament datasheet10 valuesUnless a row says otherwise: specimen not stated
Tensile modulus orientation not stated4400 MPap. 1: Tensile Modulus (ISO 527)ISO 527not in the median: set apart (never used to pass), test bar not described as printed
Tensile strength (yield or break not stated) orientation not stated50 MPap. 1: Tensile Strength (ISO 527)ISO 527not in the median: set apart (never used to pass), test bar not described as printed
Flexural modulus orientation not stated4300 MPap. 1: Flexural Modulus (ISO 178)ISO 178not in the median: set apart (never used to pass), test bar not described as printed
Flexural strength orientation not stated55 MPap. 1: Flexural Strength (ISO 178)ISO 178not in the median: set apart (never used to pass), test bar not described as printed
Charpy impact strength orientation not stated4 kJ/m2p. 1: Impact Strength, Notched (ISO 179)ISO 179not in the median: set apart (never used to pass), test bar not described as printed
HDT at 0.45 MPa58 °Cp. 1: HDT B - 0.45 MPa (ISO 75)
ISO 75As the sheet prints it: HDT B - 0.45 MPa ISO 75
not in the median: set apart (never used to pass), test bar not described as printed
HDT at 1.8 MPa54 °Cp. 1: HDT A - 1.8 MPa (ISO 75)
ISO 75As the sheet prints it: HDT A - 1.8 MPa ISO 75
not in the median: set apart (never used to pass), test bar not described as printed
Vicat softening temperature154 °Cp. 1: Vicat Softening Temperature (ISO 306)ISO 306
Melting temperature170 °Cp. 1: Melting Temperature (Tm) (DSC)DSC
Density1.35 g/cm3p. 1: Density (ISO 1183)ISO 1183

Print settings

Nozzle
190–230 °Cown data sheet
Bed
50–70 °Cown data sheet
Heated chamber
not stated
Drying
50 °C for 4–6 hown data sheet
Hardened nozzle
not stated
Its print profile, in the documents' words
What the maker says (4)
Extrudr GREENTECData sheet shared with Fabru GreenTECSold as toughened (the maker's statement)Strength XY, MPa46Modulus XY, GPa3.2Charpy notched, kJ/m²12HDT 0.45, °C—HDT 1.8, °C—Price, CAD/kg—Nozzle, °C200–230Bed, °C20–90Chamber, °CnoneDrying, °C, hnone

Extrudr GREENTECExtrudr

Data sheet shared with Fabru GreenTEC: their values are one table, recorded once.

Sold as toughened or impact-modified: "is optimised for high impact resistance" (Extrudr, TECHNICAL DATA SHEET GREENTEC, p. 1). The maker's statement, not a test result.

Published values

PropertyAs publishedConditionsOn the Overview
Extrudr, TECHNICAL DATA SHEET GREENTEC12 valuesUnless a row says otherwise: moulded bar (resin supplier's value)
Tensile modulus3200 MPap. 1: Tensile modulus (E-Modulus) ISO 527 MPaISO 527not in the median: measured on a moulded bar
Tensile strength (yield or break not stated)46 MPap. 1: Tensile strength ISO 527 MPaISO 527not in the median: measured on a moulded bar
Tensile break strength18 MPap. 1: Stress at break ISO 527 MPaISO 527not in the median: measured on a moulded bar
Elongation at break14 %p. 1: Nominal elongation at break ISO 527-2 %
ISO 527As the sheet prints it: ISO 527-2
not in the median: measured on a moulded bar
Tensile strain at strength3 %p. 1: Elongation at strenght ISO 527 %ISO 527listed under other properties
Charpy impact strength19 kJ/m2p. 1: Notched impact strength ISO 179/1eA kJ/m2
ISO 179As the sheet prints it: ISO 179/1eA
not in the median: measured on a moulded bar
Charpy impact strength218 kJ/m2p. 1: Unnotched impact strength ISO 179/1eU kJ/m2
ISO 179As the sheet prints it: ISO 179/1eU
not in the median: measured on a moulded bar
Vicat softening temperature115 °Cp. 1: VICAT A (VST) ISO 3146-C °C
ISO 3146As the sheet prints it: ISO 3146-C
Melting temperature180-200 °Cp. 1: Melting temperature ISO 1133 °Cspecimen not stated, ISO 1133
Density1.3 g/cm³p. 1: Density ISO 1183 g/cm³specimen not stated, ISO 1183
Melt mass-flow rate8 g/10minp. 1: MFR ISO 75 g/10minspecimen not stated, ISO 75
Mould shrinkage orientation not stated0.5 %p. 1: Shrinkingspecimen not stated,
ISO 294As the sheet prints it: ISO 294-4
Extrudr, GreenTEC2 valuesUnless a row says otherwise: specimen not stated; its document points to a moulded or resin bartested at 23 °C
Charpy impact strength orientation not stated12 kJ/m²p. 1: Charpy notched impact strength (+23°C)
ISO 179As the sheet prints it: ISO 179-1eA
not in the median: set apart (never used to pass), test bar not described as printed
Charpy impact strength orientation not stated228 kJ/m²p. 1: Charpy unnotched impact strength (+23°C)
ISO 179As the sheet prints it: ISO 179-1eU
not in the median: unnotched

Print settings

Nozzle
200–230 °Cown data sheet
Bed
20–90 °Cown data sheet
Heated chamber
not requiredown data sheet
Drying
not neededown data sheet
Hardened nozzle
not neededown data sheet
Its 2 print profiles, in the documents' words
  • Nozzle 200-230°C; Bed 20-90°CExtrudr, TECHNICAL DATA SHEET GREENTECp. 1: Recommended printing settings; p. 1: Hardened Nozzle; p. 1: Recommended settings for printers with a 0.4mm Nozzle
  • Nozzle 200–230 °C; Bed 20–90 °C; Drying GreenTEC does not require drying before use to achieve optimal print quality; Drying temperature 60 °C Drying time 0–4 hExtrudr, GreenTECp. 1: Print Settings; Drying
What the maker says (1)
Fabru GreenTECData sheet shared with Extrudr GREENTECStrength XY, MPa46Modulus XY, GPa3.2Charpy notched, kJ/m²12HDT 0.45, °C—HDT 1.8, °C—Price, CAD/kg—Nozzle, °C180–230Bed, °C50–90Chamber, °CnoneDrying, °C, h802 h

Fabru GreenTECFabru

Data sheet shared with Extrudr GREENTEC: their values are one table, recorded once.

Published values

PropertyAs publishedConditionsOn the Overview
Fabru, GreenTEC (purefil material data sheet)8 valuesUnless a row says otherwise:
print settingsTechnische Daten table; no specimen, print or conditioning conditions stated
Tensile modulus orientation not stated3200 MPap. 1: Zug-E-Modul (Technische Daten)ISO 527not in the median: set apart (never used to pass), test bar not described as printed
Tensile yield strength orientation not stated46 MPap. 1: Streckspannung (Technische Daten)ISO 527not in the median: set apart (never used to pass), test bar not described as printed
Elongation at break orientation not stated14 %p. 1: Reissdehnung (Technische Daten)ISO 527not in the median: set apart (never used to pass), test bar not described as printed
Elongation at yield orientation not stated3 %p. 1: Streckdehnung (Technische Daten)ISO 527listed under other properties
Vicat softening temperature115 °Cp. 1: Vicat Erweichungstemperatur A (Technische Daten)ISO 306
Density1.30 g/cm3p. 1: Dichte (Technische Daten)no standard stated
Melt volume-flow rate4 cm /10min cm3/10minp. 1: MFR (Technische Daten)ISO 1133
Mould shrinkage0.5 %p. 1: Schwindung (Technische Daten)
ISO 294As the sheet prints it: ISO 294-4, 2577

Print settings

Nozzle
180–230 °Cown data sheet
Bed
50–90 °Cown data sheet
Heated chamber
not requiredExtrudr GREENTEC's data sheet, shared
Drying
80 °C for 2 hown data sheet
Hardened nozzle
not stated
Its print profile, in the documents' words
What the maker says (11)
Fabru GreenTEC ProStrength XY, MPa50Modulus XY, GPa4.4Charpy notched, kJ/m²—HDT 0.45, °C115HDT 1.8, °C—Price, CAD/kg—Nozzle, °C190–250Bed, °C50–90Chamber, °C—Drying, °C, h802 h

Fabru GreenTEC ProFabru

Published values

PropertyAs publishedConditionsOn the Overview
Fabru, GreenTEC Pro9 values
Tensile modulus orientation not stated4400 MPap. 1: Tensile modulus (ISO 527)ISO 527not in the median: set apart (never used to pass), test bar not described as printed
Tensile yield strength orientation not stated50 MPap. 1: Yield stress (ISO 527)ISO 527not in the median: set apart (never used to pass), test bar not described as printed
Elongation at break orientation not stated3.4 %p. 1: Elongation at break (ISO 527)ISO 527not in the median: set apart (never used to pass), test bar not described as printed
Elongation at yield orientation not stated3 %p. 1: Elongation at yield (ISO 527)ISO 527listed under other properties
HDT at 0.45 MPa115 °Cp. 1: Heat deflection temperature
ISO 75As the sheet prints it: 0.45 MPa (ISO 75-2)
not in the median: set apart (never used to pass), test bar not described as printed
Vicat softening temperature160 °Cp. 1: Vicat softening temperature Ano standard stated
Density1.39 g/cm3p. 1: Densityno standard stated
Melt mass-flow rate12 g/10minp. 1: MFR (ISO 1133)ISO 1133
Mould shrinkage orientation not stated0.5 %p. 1: Shrinkage (ISO 294-4, 2577)
ISO 294As the sheet prints it: 2577 ISO 294-4

Print settings

Nozzle
190–250 °Cown data sheet
Bed
50–90 °Cown data sheet
Heated chamber
not stated
Drying
80 °C for 2 hown data sheet
Hardened nozzle
not stated
Its print profile, in the documents' words
  • Nozzle 190-250 °C; Bed 50-90 °C; Drying 80°C, 2hFabru, GreenTEC Prop. 1: Printing temperature; p. 1: Heated bed temperature; p. 1: Drying temperature / Drying time
What the maker says (6)
  • BenefitsCompared to GreenTEC, GreenTEC Pro has an increased heat resistance and is therefore particularly suitable for high-temperature applications.Fabru, GreenTEC Prop. 1
  • BenefitsGreenTEC Pro is an ecological alternative to other technical plastics, consisting of 100% renewable raw materials and biodegradable according to DIN EN ISO 14855.Fabru, GreenTEC Prop. 1
  • BenefitsGreenTEC Pro Filament can be processed particularly easily on all commercially available 3D printers.Fabru, GreenTEC Prop. 1
  • Warping and shrinkageLittle shrinkageFabru, GreenTEC Prop. 1
  • Odour and emissionsOdor freeFabru, GreenTEC Prop. 1
  • Printing adviceTemperatures similar to those of PLA are required for processing.Fabru, GreenTEC Prop. 1
Spectrum Greeny ProStrength XY, MPa53Modulus XY, GPa5.1Charpy notched, kJ/m²—HDT 0.45, °C84HDT 1.8, °C—Price, CAD/kg47Nozzle, °C190–220Bed, °C0–45Chamber, °CnoneDrying, °C, h504 h

Spectrum Greeny ProSpectrum

Published values

PropertyAs publishedConditionsOn the Overview
Spectrum, TECHNICAL DATA SHEET Greeny Pro11 valuesUnless a row says otherwise: specimen not stated
Tensile modulus orientation not stated5100 MPap. 1: Tensile modulusISO 527not in the median: set apart (never used to pass), test bar not described as printed
Tensile strength (yield or break not stated) orientation not stated53 MPap. 1: Tensile strengthISO 527not in the median: set apart (never used to pass), test bar not described as printed
Tensile yield strength orientation not stated52.5 MPap. 1: Tensile stress at yieldISO 527not in the median: another value of this product is in it
Tensile break strength orientation not stated51 MPap. 1: Tensile stress at breakISO 527not in the median: another value of this product is in it
Elongation at break orientation not stated2.2 %p. 1: Tensile strain at breakISO 527not in the median: set apart (never used to pass), test bar not described as printed
Elongation at yield orientation not stated1.95 %p. 1: Tensile strain at yieldISO 527listed under other properties
Tensile strain at strength orientation not stated1.9%p. 1: Strain at tensile strength
ISO 527As the sheet prints it: ISO 527; Mechanical Properties
listed under other properties
Charpy impact strength45 kJ/m2p. 1: Charpy Impact Strength (23°C)
ISO 179As the sheet prints it: 23°C ISO 179/1eU
tested at 23°Cunnotched
not in the median: unnotched
HDT at 0.45 MPa84 °Cp. 1: Heat Deflection Temperature 0.45mn/m2 STORAGE AND SHELF LIFE
ISO 75As the sheet prints it: 0.45mn/m2 ISO 75
not in the median: set apart (never used to pass), test bar not described as printed
Vicat softening temperature160 °Cp. 1: Vicat Softening TemperatureISO 306
Density1.34 g/cm3p. 1: Specific Gravity
ASTM D792As the sheet prints it: D 792

Print settings

Nozzle
190–220 °Cown data sheet
Bed
0–45 °Cown data sheet
Heated chamber
not requiredown data sheet
Drying
optional: 50 °C for 4 hown data sheet
Hardened nozzle
not neededown data sheet
Its 2 print profiles, in the documents' words

Price

46.9 CAD/kgits one regular price in the sample

1 listing
  • 3DJake International: 46.9 CAD/kgSpectrum GreenyPro Traffic Black, 1,75 mm / 1000 g (SKU SPC-80901)in its price; 3DJake International (European storefront) lists 29.2 EUR for 1 kg: 29.2 EUR/kg before VAT, × 1.6084 CAD per EUR (Bank of Canada, 29 Sep 2026). Used only where no Canadian shop in the sample sells the product. Shipping, duty and Canadian stock are not included.; seen 30 Sep 2026

Its 4 documents

What the maker says (13)
Spectrum GreenyHTStrength XY, MPa52Modulus XY, GPa—Charpy notched, kJ/m²—HDT 0.45, °C87HDT 1.8, °C—Price, CAD/kg—Nozzle, °C190–220Hardened nozzle neededBed, °C0–45Chamber, °CnoneDrying, °C, h454 h

Spectrum GreenyHTSpectrum

Published values

PropertyAs publishedConditionsOn the Overview
Spectrum, TECHNICAL DATA SHEET GreenyHT8 valuesThe same values also in Spectrum, 3D Printing Filament Manufacturer PRODUCT PORTFOLIO.Unless a row says otherwise: specimen not stated
Tensile modulus orientation not stated900 MPaphysically implausiblep. 1: Tensile modulus
ISO 527As the sheet prints it: ISO 527-1
not in the median: physically implausible as published
Tensile strength (yield or break not stated) orientation not stated52 MPap. 1: Tensile strength
ISO 527As the sheet prints it: ISO 527-1
not in the median: set apart (never used to pass), test bar not described as printed
Elongation at break orientation not stated4,70%p. 1: Tensile Break at Strain
ISO 527As the sheet prints it: EN ISO 527-1; Mechanical properties
not in the median: set apart (never used to pass), test bar not described as printed
Flexural modulus orientation not stated3000 MPap. 1: Flexural ModulusISO 178not in the median: set apart (never used to pass), test bar not described as printed
HDT at 0.45 MPa87 °Cp. 1: Heat Deflection Temperature 0,45 MPaalso in Spectrum, 3D Printing Filament Manufacturer PRODUCT PORTFOLIO
ISO 75As the sheet prints it: 0,45 MPa ISO 75-1
not in the median: set apart (never used to pass), test bar not described as printed
Vicat softening temperature98 °Cp. 1: VICAT Softening TemperatureISO 306
Density1,54 g/cm3p. 1: Density
ISO 1183As the sheet prints it: ISO 1183-1/A
Melt mass-flow rate20 g/10minp. 1: performance biopolymer. In terms of rigidity and MFR (190°C, 2,16kg) hardness, it significantly outperforms classic PLA
ISO 1133As the sheet prints it: 190°C 2 16kg ISO 1133
tested at 190°C

Print settings

Nozzle
190–220 °Cown data sheet
Bed
0–45 °Cown data sheet
Heated chamber
not requiredown data sheet
Drying
optional: 45 °C for 4 hown data sheet
Hardened nozzle
neededown data sheet

Differs in another document of this product, not used in deciding (a data sheet speaks before a product page, a newer edition before an older one): hardened nozzle in Spectrum, 3D Printing Filament Manufacturer PRODUCT PORTFOLIO, Spectrum, Spectrum Filaments Product Portfolio 2025 — Prografen pp28–29.

Its 4 print profiles, in the documents' words
What the maker says (14)
3DJake niceBIOStrength XY, MPa55Modulus XY, GPa—Charpy notched, kJ/m²—HDT 0.45, °C54HDT 1.8, °C—Price, CAD/kg54Nozzle, °C200–230Bed, °C0–60Chamber, °C—Drying, °C, h—

3DJake niceBIO3DJake

Published values

PropertyAs publishedConditionsOn the Overview
3DJake, Technical Data Sheet 3DJAKE niceBIO9 values
Tensile strength (yield or break not stated) orientation not stated55 MPap. 1: Tensile strengthISO 527not in the median: set apart (never used to pass), test bar not described as printed
Flexural modulus orientation not stated5100 MPap. 1: Flexural modulusISO 527not in the median: set apart (never used to pass), test bar not described as printed
Charpy impact strength orientation not stated43 kJ/ m²p. 1: Impact strength
ISO 179As the sheet prints it: ISO 179-1/1eA
not in the median: notch not stated
HDT at 0.45 MPa54 °Cp. 1: HDT / B
ISO 75As the sheet prints it: HDT B ISO 75
not in the median: set apart (never used to pass), test bar not described as printed
Vicat softening temperature146 °Cp. 1: VICAT AISO 306
Melting temperature190 °Cp. 1: Melting temperature
ISO 3146As the sheet prints it: ISO 3146-C
Density1,33 g/ccp. 1: Specific gravityISO 1183
Melt mass-flow rate7 g/10 minp. 1: MFR 210 °C/2,16kg
ISO 1133As the sheet prints it: 210 °C/2 16kg ISO 1133
tested at 210°C
Mould shrinkage orientation not stated0,4 %p. 1: Shrinking
ISO 294As the sheet prints it: ISO 294-4

Print settings

Nozzle
200–230 °Cown data sheet
Bed
0–60 °Cown data sheet
Heated chamber
not stated
Drying
not stated
Hardened nozzle
not stated
Its 2 print profiles, in the documents' words

Price

53.6 CAD/kgits one regular price in the sample

1 listing
  • 3DJake International: 53.6 CAD/kg3DJAKE niceBIO Black, 1,75 mm / 750 g (SKU CLP-NICEBIO-BLACK-0750-175)in its price; 3DJake International (European storefront) lists 25 EUR for 0.75 kg: 33.3 EUR/kg before VAT, × 1.6084 CAD per EUR (Bank of Canada, 29 Sep 2026). Used only where no Canadian shop in the sample sells the product. Shipping, duty and Canadian stock are not included.; seen 30 Sep 2026

Its 3 documents

What the maker says (18)
Extrudr GREENTEC PROSold as toughened (the maker's statement)Strength XY, MPa—Modulus XY, GPa—Charpy notched, kJ/m²—HDT 0.45, °C—HDT 1.8, °C—Price, CAD/kg75Nozzle, °C210–230Bed, °C20–90Chamber, °CnoneDrying, °C, hnone

Extrudr GREENTEC PROExtrudr

Sold as toughened or impact-modified: "built-in flexibility for improved impact resistance" (Extrudr, GreenTEC Pro, p. 1). The maker's statement, not a test result.

Published values

PropertyAs publishedConditionsOn the Overview
Extrudr, TECHNICAL DATA SHEET GREENTEC PRO12 valuesUnless a row says otherwise: moulded bar (resin supplier's value)
Tensile modulus4300 MPap. 1: Tensile modulus (E-Modulus) ISO 527 MPaISO 527not in the median: measured on a moulded bar
Tensile strength (yield or break not stated)58 MPap. 1: Tensile strength ISO 527 MPaISO 527not in the median: measured on a moulded bar
Tensile break strength53 MPap. 1: Stress at break ISO 527 MPaISO 527not in the median: measured on a moulded bar
Tensile strain at strength2.8 %p. 1: Elongation at strenght ISO 527 %ISO 527listed under other properties
Charpy impact strength4 kJ/m2p. 1: Notched impact strength ISO 179/1eA kJ/m2
ISO 179As the sheet prints it: ISO 179/1eA
not in the median: measured on a moulded bar
Charpy impact strength71 kJ/m2p. 1: Unnotched impact strength ISO 179/1eU kJ/m2
ISO 179As the sheet prints it: ISO 179/1eU
not in the median: measured on a moulded bar
HDT at 0.45 MPa115 °Cp. 1: HDT/B ISO 75 °C
ISO 75As the sheet prints it: HDT B ISO 75
not in the median: measured on a moulded bar
Vicat softening temperature160 °Cp. 1: VICAT A (VST) ISO 306 °CISO 306
Melting temperature180-200 °Cp. 1: Melting temperature ISO 3146-C °Cspecimen not stated,
ISO 3146As the sheet prints it: ISO 3146-C
Density1.35 g/cm³p. 1: Density ISO 1183 g/cm³specimen not stated, ISO 1183
Melt mass-flow rate9 g/10minp. 1: MFR ISO 1133 g/10minspecimen not stated, ISO 1133
Mould shrinkage orientation not stated0.4 %p. 1: Shrinkingspecimen not stated,
ISO 294As the sheet prints it: ISO 294-4
Extrudr, GreenTEC Pro2 valuesUnless a row says otherwise: specimen not stated; its document points to a moulded or resin bartested at -30 °C
Charpy impact strength orientation not stated3 kJ/m²p. 1: Charpy notched impact strength (-30°C)
ISO 179As the sheet prints it: ISO 179-1eA
not in the median: tested below room temperature
Charpy impact strength orientation not stated55 kJ/m²p. 1: Charpy unnotched impact strength (-30°C)
ISO 179As the sheet prints it: ISO 179-1eU
not in the median: unnotched
Extrudr, Material Safety Data Sheet: GREENTEC PRO2 valuesUnless a row says otherwise: specimen not stated
Melting temperature190-210°Cp. 3: MELTING RANGEno standard stated
Density1.39g/cm³p. 3: DENSITYno standard stated

Print settings

Nozzle
210–230 °Cown data sheet
Bed
20–90 °Cown data sheet
Heated chamber
not requiredown data sheet
Drying
not neededown data sheet
Hardened nozzle
not neededown data sheet
Its 2 print profiles, in the documents' words
  • Nozzle 210-230°C; Bed 20-90°CExtrudr, TECHNICAL DATA SHEET GREENTEC PROp. 1: Recommended printing settings; p. 1: Hardened Nozzle; p. 1: Recommended settings for printers with a 0.4mm Nozzle
  • Nozzle 210–230 °C; Bed 20–90 °C; Drying GreenTEC Pro does not require drying before use to achieve optimal print quality; Drying temperature 60 °C Drying time 0–4 hExtrudr, GreenTEC Prop. 1: Print Settings; Drying

Price

75.4 CAD/kgits one regular price in the sample

1 listing
  • 3DJake International: 75.4 CAD/kgExtrudr Green-TEC PRO Black, 1.75 mm / 800 g (SKU EX-9010241426027)in its price; 3DJake International (European storefront) lists 37.5 EUR for 0.8 kg: 46.9 EUR/kg before VAT, × 1.6084 CAD per EUR (Bank of Canada, 29 Sep 2026). Used only where no Canadian shop in the sample sells the product. Shipping, duty and Canadian stock are not included.; seen 30 Sep 2026

Its 4 documents

What the maker says (1)

Not published by any product: tensile strength (Z).

Values are for the colour each sheet tested; pigment can change them.